Silver Maple wood movement, board-foot & weight calculator

hardwood

Handbook listing: Maple, silver

Janka
700lbf
Density
32.8lb/ft³
T/R ratio
2.4
Spec. gravity
0.47

Silver Maple is a North American hardwood. It has a Janka side hardness of 700 lbf, a specific gravity of 0.47, and an air-dry density near 33 lb/ft³ (525 kg/m³) (mechanical values at 12% moisture content). It shrinks 7.2% tangentially and 3% radially from green to oven-dry (T/R ratio 2.4), so a 12-inch flatsawn board moves about 0.17 in (≈ 3/16 in) across a 6-point moisture swing (about 6%→12% MC).

Compute Silver Maple: movement, weight & board footage

Every number below is worked from Silver Maple's own shrinkage and density figures, not looked up from a table — change the width, moisture swing, or board size in the calculators linked alongside.

Cross-grain movement by board width

Cross-grain change for a 6-point moisture swing (≈ 6%→12% MC), using ΔD = D × (S ÷ 30 ÷ 100) × ΔMC.
Board width Flatsawn (tangential) Quartersawn (radial)
2″ 0.029″ (≈ 1/32 in) 0.012″ (≈ 0 in)
3″ 0.043″ (≈ 1/32 in) 0.018″ (≈ 1/32 in)
4″ 0.058″ (≈ 1/16 in) 0.024″ (≈ 1/32 in)
6″ 0.086″ (≈ 3/32 in) 0.036″ (≈ 1/32 in)
8″ 0.115″ (≈ 1/8 in) 0.048″ (≈ 1/16 in)
10″ 0.144″ (≈ 5/32 in) 0.06″ (≈ 1/16 in)
12″ 0.173″ (≈ 3/16 in) 0.072″ (≈ 1/16 in)
16″ 0.23″ (≈ 7/32 in) 0.096″ (≈ 3/32 in)

Need a different width or moisture swing? Run the movement calculator preloaded with Silver Maple. At a T/R ratio of 2.4, Silver Maple is moderately unstable — it moves substantially more tangentially than radially, so flatsawn stock is noticeably cup-prone and quartersawn stock is worth the extra cost in wide panels.

Board footage & weight, standard sizes

8-foot lengths at Silver Maple's air-dry density of 32.8 lb/ft³ (12% MC).
Nominal size × length Board feet Weight
1×4 × 8′ 2.67 bd ft 7.3 lb
1×6 × 8′ 4 bd ft 10.9 lb
1×8 × 8′ 5.33 bd ft 14.6 lb
1×10 × 8′ 6.67 bd ft 18.2 lb
1×12 × 8′ 8 bd ft 21.9 lb
2×4 × 8′ 5.33 bd ft 14.6 lb
2×6 × 8′ 8 bd ft 21.9 lb
2×8 × 8′ 10.67 bd ft 29.2 lb

Different length or size? Run the board foot calculator or the weight calculator, both preloaded with Silver Maple.

Seasonal movement by city

Width change of a 12″ flatsawn board between each city's driest and most-humid month, from USDA equilibrium-moisture-content data.
City Driest month (EMC) Most-humid month (EMC) EMC swing 12″ board movement
Phoenix, AZ Jun · 4.4% Dec · 9% 4.6 pts 0.132″ (≈ 1/8 in)
Chicago, IL May · 12.3% Dec · 15.1% 2.8 pts 0.081″ (≈ 3/32 in)
Miami, FL Apr · 12.2% Sep · 14.4% 2.2 pts 0.063″ (≈ 1/16 in)
Boston, MA Apr · 11.5% Sep · 12.8% 1.3 pts 0.037″ (≈ 1/32 in)
Denver, CO Jul · 8% Dec · 10.5% 2.5 pts 0.072″ (≈ 1/16 in)
Seattle, WA Jul · 12% Dec · 16.9% 4.9 pts 0.141″ (≈ 5/32 in)

Driven by Silver Maple's tangential shrinkage of 7.2%. These are outdoor equilibrium-moisture figures, so they are an upper bound — a climate-controlled interior swings less. How this is calculated.

How Silver Maple compares

Ranked against the 196 species in the Wood Handbook tables this site carries.

See Silver Maple plotted against every species we carry: the full Janka hardness chart and the full density chart .

Species with a similar working profile

Closest matches on hardness, weight and stability together — useful when Silver Maple is unavailable or priced out.

Species Janka Density T/R
Teak 1,000 lbf 38.4 2.32

About Silver Maple

The Wood Handbook describes Silver Maple as part of the Maple (Soft Maple Group); the account below is of that group, which Silver Maple belongs to.

Soft maple includes silver maple (Acer saccharinum), red maple (A. rubrum), boxelder (A. negundo), and bigleaf maple (A. macrophyllum). Silver maple is also known as white, river, water, and swamp maple; red maple as soft, water, scarlet, white, and swamp maple; boxelder as ash-leaved, three-leaved, and cut-leaved maple; and bigleaf maple as Oregon maple. Soft maple is found in the eastern United States except for bigleaf maple, which comes from the Pacific Coast. Heartwood and sapwood are similar in appearance to hard maple. Sapwood of soft maple is somewhat lighter in color than the heartwood. The wood of soft maple, primarily silver and red maple, resembles that of hard maple but is not as heavy, hard, and strong. Soft maple is used for railroad crossties, boxes, pallets, crates, furniture, veneer, wooden ware, and novelties.

Wood Handbook, Chapter 2: Characteristics and Availability of Commercially Important Woods (M.C. Wiemann), USDA Forest Products Laboratory, FPL-GTR-282 (2021), p. 9. Public domain.

Durability & sustainability

CITES status: not listed on any CITES Appendix — no international-trade restriction applies to Silver Maple.

Properties

At 12% moisture content unless noted.
Specific gravity 0.47
Janka hardness (side) 700 lbf
Density (air-dry, 12% MC) 32.8 lb/ft³ (525 kg/m³) ovendry-weight basis: 29.3 lb/ft³
Weight per board foot (air-dry) 2.73 lb
Radial shrinkage (green→oven-dry) 3%
Tangential shrinkage (green→oven-dry) 7.2%
Volumetric shrinkage (green→oven-dry) 12%
T/R ratio (stability indicator) 2.4

Shrinkage is total green-to-oven-dry (Table 4-3); strength values are at 12% MC. Full bases and the derivation formulas are on the methodology page.

Data: USDA Forest Products Laboratory, Wood Handbook FPL-GTR-282 (2021), public domain.